Bolting Data
Design Stress Values (ksi) vs Temperature
| SPEC | GRADE | TEMPERATURE deg F (deg C) | |||||||||
| 650 | 700 | 750 | 800 | 850 | 900 | 950 | 1000 | 1050 | 1100 | ||
| (343) | (371) | (399) | (427) | (454) | (482) | (510) | (538) | (566) | (593) | ||
| ASTM A193 | B6 |
21.2 | 21.2 | 21.2 | 19.5 | 15.6 | 12.0 | ||||
ASTM A193 ASTM A193 ASTM A193 ASTM A193 ASTM A193 |
B7 (*) B7M (*) B8-CL1 B8-CL2 (**) B16 |
25.0 20.0 11.2 25.0 25.0 |
25.0 20.0 11.0
25.0 |
23.6 20.0 10.8
25.0 |
21.0 18.5 10.5
25.0 |
17.0 16.2 10.3
23.5 |
12.5 12.5 10.1
20.5 |
8.5 8.5 9.9
16.0 |
4.5 4.5
11.0 |
6.3 |
2.8 |
| ASTM A320 | L7 | 25.0 | 25.0 | ||||||||
| BS | B17B | 20.0 | 19.8 | 19.8 | 19.8 | 19.7 | 19.7 | 19.6 | 19.4 | 19.3 | 16.6 |
| ASTM 453 | 660 | 20.2 | 20.1 | 20.0 | 19.9 | 19.9 | 19.9 | 19.8 | 19.8 | ||
Recommended working temperatures of bolt materials
| MATERIAL | TEMPERATURE °C (°F) | |||||||||
| MIN. | MAX. | |||||||||
CARBON STEEL B7, L7 B6 B8 B16 B17B INC 718 660 |
-29 (-20) -73 (-100) 0 (32) -200 (-325) 0 (32) -29 (-20) 0 (32) -29 (20) |
300 (572) 400 (752) 500 (932) 575 (1067) 520 (968) 650 (1202) 750 (1382) 538 (1000) |
||||||||
All dan-loc stud bolts are quenched and tempered
ASTM A - 194 "Standard Specification for Carbon and Alloy Steel Nuts for Bolts for High-Pressure and High-Temperature Service"
| Identification | AISI Type | Outstanding Chemical |
| Ferritic | ||
| L-7 | 4140-4142-4145 | Chromium-Moylbdenum |
| L-7M | 4140-4142-4145 | Chromium-Molybdenum |
| L-7A | 4037 | Carbon-Molybdenum |
| L-7B | 4137 | Chromium-Molybdenum |
| L-7C | 8740 | Nickel-Chromium-Molybdenum |
| L-43 | 4340 | Nickel-Chromium-Molybdenum |
| Austenitic | ||
| B8, B8A | 304 | Unstabilized 18 Chromium-8 Nickel |
| B8-C, B8CA | 347 | Stabilized 18 Chromium-8 Nickel |
| B-8M, B8MA | 316 | 18 Chromium-10-Nickel-2 Molybdenum |
| B-8T, B8TA | 321 | Stabilized 18 Chromium Nickel |
| B-8F, B8FA | 303 | Free Machining 18 Chromium-8 Nickel |
The Ferritic Steel Grades L7 and L7M together with the Austenitic Grades B8 and B8M are normally stocked for immediate shipment, with the other Grades available on special order. Grade L7 is normally used to -50°F without a Charpy Test and to -150°F with a Charpy Test. Grade L7M is normally used in H2S service with a required Charpy Test at -100°F. All of the Austenitic steels listed above may be used to -325°F without a Charpy Impact Test and at lower temperatures with the requisite Impact Tests.
ASTM A - 320 "Standard Specification for Alloy-Steel and Stainless-Steel Bolting Materials for Low-Temperature Service"
| Identification | AISI Type | Outstanding Chemical |
| Ferritic | ||
| 2-HM | Carbon |
|
| 2-H | Carbon | |
| 4 | Carbon-Molybdenum | |
| 3 | 501 | 5% Chromium |
| 6 | 410 | 12% Chromium |
| 6-F | 416 | 12% Chromium |
| 7 | 4140-4142-4145 | Chromium-Molybdenum |
| Austenitic | ||
| 8 | 304 | 18 Chromium-8 Nickel |
| 8-C | 347 | 18 Chromium-8 Nickel |
| 8-M | 316 | 18 Chromium-10-Nickel-2 Molybdenum |
| 8-T | 321 | 18 Chromium-8 Nickel |
| 8-F | 303 | 18 Chromium-8 Nickel |
| 8-P | 305 | 18 Chromium-10 Nickel |
DAN-LOC stocks the Ferritic steel nuts in Grades 2H, 2HM, 7, L7, and L7M which are normally used in conjunction with Grade B7, B7M, B16, L7 and L7M studs. The Austenitic steel nuts, Grade 8 and 8M are also available from stock for use on stainless steel studs and bolts. DAN-LOC stocks heavy pattern hex nuts in the grades listed above to the dimensional requirements of ANSI B18.22.1. Unless otherwise specified, these nuts are tapped UNC-2B in sizes 1" and under, and 8UN-2B over 1" diameter. All other grades of nuts listed may require special order.
725 North Drennan
Houston, Texas 77003-1320
Telephone: 713-356-3560
Toll Free: 1-800-231-6355
Email DLX Texas
20444 Tillman Ave
Carson, California 90746
Telephone: 310-438-4320
Toll Free: 1-800-682-2658
Email DLX California
1345 Taylor Farm Road
Suite 110
Virginia Beach, Virginia 23453
Telephone: 757-468-1781
Email DLX Virginia
#29825 - 44 Avenue
Edmonton, Alberta, Canada
T6E 5E3
Telephone: 780-701-0524
Email DLX Canada